Abstract
In this letter we report the effect of CuO and MnO2 additives on the sintering behavior of 0.95(Na0.5K0.5)NbO3-0.05BaTiO3 ceramics. It was found that the composition corresponding to 0.95(Na0.5K0.5)NbO3-0.05BaTiO3 + 2.0 mol% CuO + 0.5 mol% MnO2, sintered at 950 °C for 10 h, exhibited excellent piezoelectric properties corresponding to: kp = 0.41, d33 = 248 pC/N, Qm = 305, ε3T/ε0 = 1258, and Tc = 280 °C. These results indicate the prominence of this composition in lead-free systems.
Original language | English |
---|---|
Pages (from-to) | 3594-3596 |
Number of pages | 3 |
Journal | Materials Letters |
Volume | 62 |
Issue number | 20 |
DOIs | |
Publication status | Published - 2008 Jul 31 |
ASJC Scopus subject areas
- Materials Science(all)
- Condensed Matter Physics
- Mechanics of Materials
- Mechanical Engineering